Six numbers define the spring, and one of them is a direction
A torsion spring is fully described by wire diameter d, mean coil diameter D (or outside diameter plus d), total body coils nk, leg geometry, the torque required at two defined angular positions, and the winding direction. Leave any of them out and the factory fills the gap with what is on the machine that week.
Spring index w = D/d is the number behind the first one. The workable band is 4 to 12, and 5 to 8 is where coiling is stable, curvature stress is moderate and the body does not buckle. Below 4 the wire is difficult to wind and the inner-fibre stress rises sharply; above 12 the body distorts under load and the legs lose their angular position.
Winding direction is the note that causes the most field failures. A torsion spring must be loaded in the direction that winds the coil up — tightening it, reducing the body diameter. Loaded the other way the body opens, the diameter grows, any preset residual stress is lost, and fatigue life drops. State RH or LH explicitly and mark the load direction with an arrow on the drawing.
Torque, rate and stress: the maths worth checking yourself
Rate follows the bending stiffness of the wire: θ in revolutions = 10.19 · M · D · n / (E · d⁴), with M in N·mm, D and d in mm, E = 206,000 N/mm² for spring steel, and n the number of active coils. The legs are active material too, so n is larger than the body count — the DIN 2097 convention adds them as (l1 + l2) / (3πD) equivalent coils. A 40 mm pair of legs on a Ø16 mm mean diameter adds about 0.27 coils, which is 3-4% of rate on a short body.
Stress is the number that decides life. Nominal bending stress in the body is σ = 32·M / (π·d³), and the inner fibre is worse than that because of curvature, so multiply by the Wahl-type factor q = (4w² − w − 1) / (4w(w − 1)), which gives about 1.10 at index 8 and 1.23 at index 5.
Worked example: d = 2.0 mm, D = 16 mm (index 8), 8.25 body coils, EN 10270-1-SH wire with Rm 1,520-1,720 N/mm². Rate ≈ 2,450 N·mm per revolution, or about 6.8 N·mm per degree. At 500 N·mm the nominal stress is 637 N/mm² and the corrected inner-fibre stress is roughly 700 N/mm² — about 45% of the lower tensile limit. Comfortable for static duty; for a million cycles it needs shot peening and a lower working stress.
Why the legs crack and the body survives
The body is cold-worked during coiling and carries beneficial residual stress; the legs are straight wire that never got that treatment, and they end at the coil-to-leg transition, which is a sharp bend with a small radius. A tight transition radius gives a stress concentration factor of two to three or more, on top of a nominal stress that is already highest where the leg leaves the body.
Then the assembly adds to it. A load applied at the leg tip rather than near the seat puts an extra bending moment into the root. Fretting against a housing or a pivot pin initiates cracks that no material change will fix. Over-travel is the worst one: once the coils go solid, rate goes to infinity and every additional degree of rotation is absorbed by the legs, so a mechanism that jams at the end of its stroke breaks legs, not bodies.
Material and process causes account for the rest. Seams and laps in the wire are classic origins, which is why EN 10270-1 requires a surface free of them and patented, tempered wire rather than anything redrawn from stock. Hydrogen embrittlement after electroplating cracks high-tensile wire within days, not months. And corrosion pits under cyclic stress reduce the fatigue limit by a third to a half — a rusted torsion spring in a damp enclosure is a fatigue problem wearing a cosmetic one.
Preload, travel and the bind point
Specify preload as a torque at an angle, not as an adjective: M1 = 180 N·mm at the installed position θ1 = 30° from free, M2 = 420 N·mm at full travel θ2 = 120°, free angle between legs 90° ± 3°. Two points define the curve and let the supplier check both rate and initial tension; one point does not, and a spring can hit a single-point spec with the wrong rate.
Ask for the coil-bind angle and put a mechanical stop in the housing that engages before it. The body diameter shrinks as the spring winds up, so also check the free inside diameter against the mandrel: allow 0.2-0.5 mm diametral clearance on small springs and more where travel exceeds 90°, or the body will close onto the shaft and bind.
Tolerances should be stated as a grade. DIN 2098 defines tolerance grades 1, 2 and 3 for cold-coiled torsion springs; leg angular position is typically held to ±2° to ±5° depending on leg length and grade, and torque to about ±10% at grade 2, with ±5-8% achievable when the wire is sorted and the first article is measured. Tolerance grade 1 on a 40 mm leg costs more than the spring is worth — say which dimensions are functional and let the rest go to grade 3.
Cycle life: stress relief, presetting and shot peening
Stress relief after winding is the cheapest life insurance there is: typically 250-350 °C for 20-40 minutes depending on wire type, which removes coiling residual stress without softening the material. It should be on the process route, not left to the shop discretion, and austenitic and precipitation-hardening stainless wires have their own temperature windows.
Presetting (over-winding the spring past its working angle) sets the free angle and leaves favourable compressive residual stress in the surface. Shot peening does the same thing more thoroughly and is what separates a 10⁵-cycle part from a 10⁶-cycle part — typical gains are two to five times life at the same stress range. Specify it properly: Almen intensity around 0.10-0.25 mm A and coverage of at least 100%, peened after winding and before any coating, and not on wire below roughly 0.5 mm where the peening distorts the geometry.
Then ask for evidence. A fatigue test on a cyclic rig to the specified cycle count at the specified torque range, with the recorded count and the fracture location if it fails, is worth more than any calculation. State the target as a number: 10⁵, 10⁶ or 10⁷ cycles, at M1 to M2, in the specified environment.
Wire, finish and the plating trap
EN 10270-1 covers patented cold-drawn unalloyed spring wire in classes SM (static), SH (high stress static and dynamic), DM and DH, with DH being the normal choice for dynamic duty; Rm scales with diameter, so a 2.0 mm SH wire is around 1,520-1,720 N/mm² and a 6.0 mm wire of the same class is roughly 1,270-1,470 N/mm². EN 10270-2 covers stainless (302, 304, 316, 17-7 PH) and EN 10270-3 corrosion-resistant non-ferrous wire. Chrome-silicon 55CrSi and oil-tempered 5160 suit larger sections and shock duty; nickel superalloy X-750 and Co-Ni-Cr alloy are the high-temperature answers.
Finish is where high-strength wire gets destroyed. Any electroplated wire above roughly 1,000 N/mm² Rm or 32 HRC needs a hydrogen bake within four hours of plating — 190-220 °C for four to eight hours per ISO 9588 or ASTM B850 — and a bake that happens the next morning is not a bake. Where the shop cannot guarantee it, specify a hydrogen-free process instead: mechanical plating, or zinc flake coating to ISO 10684, which also gives 480-1,000 hours of neutral salt spray per ISO 9227 against 72-96 hours for plain zinc.
Stainless is not automatically better. Austenitic 304 has a lower strength than SH wire and work-hardens unpredictably, so a carbon-steel spring with the right coating often beats it on fatigue in a dry enclosure, while 316 or 17-7 PH wins in wet, washdown or marine duty. State the environment, the temperature range and the number of cycles, and let the material follow.
The drawing annotations that prevent the failure
Minimum set: material and wire standard with class and diameter tolerance (EN 10270-1-SH, Ø2.00 h11); mean diameter or outside diameter with tolerance; total body coils ± 1/4; free angle between legs with tolerance; leg lengths, bend radii (minimum 1×d at the transition, 2-3×d better) and the load application point on each leg; winding direction RH or LH with a load-direction arrow.
Second block: torque at two angular positions with the maximum working angle and the coil-bind angle stated separately; presetting required yes or no; shot peening with Almen intensity and coverage; stress relief temperature and time; finish, coating thickness, salt-spray hours to ISO 9227 and, if electroplated, the hydrogen bake requirement; surface condition note requiring wire free of seams, laps and decarburisation per EN 10270-1.
Third block, and the one that stops drift: first-article requirement with a measured torque-angle curve and actual values at both specified angles attached to the approval, packing that prevents leg distortion (nested on a mandrel, in trays or oriented in bags), and a note that the drawing revision governs over the sample. Keep the approved first article and its curve on file — it is the reference every reorder is judged against, and it is the only thing that stops the rate creeping two batches later.
Questions this guide raises
What information is needed to quote a torsion spring?
Wire material and diameter, mean or outside coil diameter, total body coils, leg lengths and the angle between them, winding direction, torque at two angular positions, maximum travel, cycle-life target, finish and quantity. A physical sample or a photo with a scale works when the numbers are unknown, and a first article is measured back into a drawing.
How many cycles can a torsion spring be designed for?
Static and low-cycle duty is essentially unlimited at stresses under about 45-50% of Rm. For 10⁵ cycles, stress relief, presetting and a leg transition radius of at least 1×d are normally enough. For 10⁶ to 10⁷ cycles, add shot peening with a stated Almen intensity and coverage, reduce the working stress range, and validate on a cyclic rig with a recorded count.
Why did the legs crack while the body was fine?
Because the leg root combines the highest bending moment with a sharp transition radius, un-work-hardened straight wire and often an off-axis or over-travelled load. Once the coils go solid, all additional rotation is absorbed by the legs. Fix it with a larger transition radius, a load applied near the seat, a mechanical stop before bind, and shot peening.
Can we drop shot peening to save cost?
Only on static or low-cycle applications. In dynamic duty the peening step is usually a small single-digit percentage of piece cost and buys a multiple of fatigue life, so removing it is the most expensive saving available. If the budget is the constraint, reduce the working stress by increasing wire diameter instead and quote both options.