When wear is the problem, not weather. Type II is the ordinary sulfuric anodic coating, typically 5-25 µm, takes dye well and is the standard answer for appearance and general protection. Type III is the hard-coat family: dense, commonly 25-75 µm, markedly harder, chosen for abrasion, galling and dielectric duty - and it takes colour badly. The thickness range is the specification; the type word alone is not one.
About half the coating grows outward, so a 50 µm hard coat adds some 25 µm to an outside dimension and closes a bore by a similar amount. That is why dimensions are stated after treatment, why a 0.1 mm clearance between pin and bore can vanish when both surfaces take a hard coat, and why threads are masked or re-tapped. Thickness is checked with a magnetic or eddy-current gauge, or destructively by the ASTM B137 weigh-back method.
The alloy and the sealing decide the rest. Designations are described by practices such as ASTM B580 and classified by value bands in ISO 7599, with the EN 12373 series covering the anodising tests - and a coating is only as good as its seal, because a porous unsealed layer adsorbs stains and dye. High-copper 2xxx and most cast alloys anodise poorly, anodic coatings cost a little fatigue strength, and they are dielectric, so grounding pads must be masked.
The two families side by side - thickness and hardness claims belong on the drawing as ranges with a measurement method, not as a type word| Attribute | Type II (standard anodic) | Type III (hard anodic) | What to write on the drawing |
|---|
| Coating thickness | commonly 5-25 µm, with architectural use pushing the upper bands | commonly 25-75 µm and sometimes more | a thickness range plus the gauge method and the sample basis |
|---|
| Hardness and wear | soft enough to mark in handling; modest abrasion resistance | dense and much harder, specified against scuffing and wear | the wear or galling requirement, since the value varies with alloy and bath |
|---|
| Dimension change | a few micrometres per surface - usually ignorable at 10 µm | roughly half the coating stands proud, so fits shift measurably | all dimensions after treatment, with the masked features listed |
|---|
| Appearance and dyeing | takes dye well; colour match needs batch and current control | low uptake, typically grey through to dark, colour is unreliable | a colour standard and a light-fastness requirement if colour is functional |
|---|
| Sealing | hot deionised water or steam, or a cold nickel-fluoride seal | same requirement, and an unsealed hard coat stains readily | the sealing method and its verification test from the EN 12373 series |
|---|
| Corrosion behaviour | the normal outdoor answer on 5xxx and 6xxx when sealed | thicker barrier but not a substitute for a paint system in aggressive exposure | the exposure category and the required chamber test, if one is required |
|---|
| Alloy response | 6xxx and 5xxx anodise cleanly; 2xxx goes grey and less protective | hard coat on high-copper and cast alloys is patchy and variable | the alloy number next to the finish requirement, never the finish alone |
|---|
Values are the published minima, maxima or bands of the standards named in the table, taken at the stated thickness, size or temperature. Where a standard tabulates a value by size band, the value for your goods comes from the mill or test certificate, which we attach to the quotation instead of summarising it here.