Xingtai, Hebei · Hebei industrial clusters

Specification reference · updated 29 September 2026

Are 42CrMo4, 4140 and SCM440 the same quenched and tempered alloy steel?

Close, not identical. All three are chromium-molybdenum medium-carbon steels at 0.37-0.45 % carbon with 0.9-1.2 % chromium and about 0.2 % molybdenum, so a drawing calling for one can usually be filled by another in the same heat-treated condition. The real gap is hardenability and the standard the certificate is written against, and that gap only bites above roughly 80 mm of section.

Close, not identical. All three are chromium-molybdenum medium-carbon steels at 0.37-0.45 % carbon with 0.9-1.2 % chromium and about 0.2 % molybdenum, so a drawing calling for one can usually be filled by another in the same heat-treated condition. The real gap is hardenability and the standard the certificate is written against, and that gap only bites above roughly 80 mm of section.

42CrMo4 is the EN 10083-2 grade, 4140 is the SAE J402 designation with bar commonly bought to ASTM A29, and SCM440 is JIS G4105. Their chemistry bands overlap almost completely. What differs is the condition the bar is delivered against: EN material arrives in a named condition (+A annealed, +QT quenched and tempered) with an EN 10204 3.1 certificate.

What goes wrong is the substitute nobody checks. GB/T 3077 40Cr has chromium but no molybdenum, so it hardens shallowly and loses temper resistance sooner; it is not a 42CrMo4. For a shaft, rod or die block above 80 mm, or anything that runs hot, name the condition and the core hardness on the drawing, not only the grade number.

Chemistry bands for the three chromium-molybdenum grades (mass %, as published in each standard)
Element or property42CrMo4 (EN 10083-2)4140 (SAE J402 / ASTM A29)SCM440 (JIS G4105)
Carbon0.38-0.450.38-0.430.37-0.44
Chromium0.90-1.200.80-1.100.90-1.20
Molybdenum0.15-0.250.15-0.250.15-0.30
Manganese0.60-0.900.60-0.900.60-0.90
Maximum hardness, annealed bar255 HB255 HB annealed band255 HB
Practical through-hardening on oil quenchabout Ø80-110 mm, section-dependentabout Ø80-100 mmabout Ø70-100 mm
Typical welding preheat200-250 °C, low-hydrogen process200-250 °C, low-hydrogen process200-250 °C, low-hydrogen process

Values are the published minima, maxima or bands of the standards named in the table, taken at the stated thickness, size or temperature. Where a standard tabulates a value by size band, the value for your goods comes from the mill or test certificate, which we attach to the quotation instead of summarising it here.

Where this costs money

Three situations where the difference becomes a claim

Each is a decision taken at quotation stage, while the specification is still cheap to change.

The section is over about 80 mm and the property is required at the core

Hardenability decides whether the middle of the bar transforms at all. The slightly higher carbon and chromium give 42CrMo4 more depth than 4140 or SCM440 in the same diameter. Ask for a hardness traverse across the section or a Jominy end-quench record; the letters QT on a delivery note prove nothing about the core.

The drawing says 40Cr and you are offered 42CrMo4

The two numbers sit next to each other in a cross-reference table and are not the same steel. Without molybdenum the hardening depth and the strength at tempering temperature are lower, so the substitution must be raised as a deviation with the reason written down, not delivered silently because a conversion chart said similar.

You are nitriding or induction hardening after machining

The supply condition must be tempered above the final treatment temperature or the core softens and the part moves when it is nitrided. For a 500-570 °C nitriding cycle that means a tempering temperature comfortably above it, stated in the purchase order and confirmed on the certificate - a detail that gets lost between the drawing and the bar supplier.

Questions buyers ask before they commit the specification

Which is stronger, 42CrMo4 or 4140?

Tempered to the same hardness they are comparable. The difference appears in large sections: 42CrMo4 carries marginally more carbon and chromium, so it hardens deeper and keeps more strength at the core of a thick bar. As a general which-grade-is-stronger statement the question has no answer, because the heat-treated condition does the work.

Can I get EN 10204 3.1 certificates with an SAE grade?

Yes. The certificate system follows the purchase order, not the name of the grade. We order 3.1 inspection with heat number, chemistry, and hardness or tensile results for the stated condition, plus ultrasonic class where the section requires it. Specify it in the enquiry and the price reflects it.

Should rough-turned bar arrive annealed or already quenched and tempered?

Both routes are legitimate and they cost differently. Annealed bar lets you machine and then heat treat, which means distortion and scale to allow for. Quenched-and-tempered bar machine-finishes closer to size but softens wherever it is welded locally and is harder on tooling. Decide with the shop against the drawing before the order is placed.

Is SCM440 simply the Japanese 4140?

The chemistry bands are nearly identical and in practice they fill the same role. SCM440 is delivered to JIS G4105 with JIS testing (hardness and, when required, JIS G1201 end-quench hardenability), while 4140 is delivered to SAE and ASTM. Accept either with the condition and test package named; do not accept the phrase 4140 equivalent with no condition at all.

Fit this to a real part

Send the drawing and the answer comes back with your numbers

The quotation for forged parts & rings repeats this comparison against your grade, dimension, tolerance and test package, and names any deviation before production starts.

Ask about this specificationForged Parts & Rings category hub

How we verify it

  • Grade and condition checked against the EN 10204 3.1 certificate and the heat marking.
  • Boundary dimensions, class, clearance or rating measured on the inspection sheet.
  • Deviations offered in writing before production, never discovered after shipment.

Trading and sourcing company based in northern Xingtai, Hebei, about 60 km south of the provincial capital. We buy across the industrial clusters of central and southern Hebei and reach the northern ones on scheduled factory runs; the supplier visits, benchmarking and pre-shipment inspection are ours, done in person. Not a factory. Multi-category, quoted from drawings, consolidated into one container and one document pack, and inspected before the balance is paid; every order starts as an RFQ.

Inspection and documents →

Written first reply within 1 working day; priced answer within 2-5 working days.

Quote it against your part, not the chart

Send the drawing, the standard your engineer named and the quantity. We reply with the priced specification, the substitution we recommend and why, and the inspection plan that proves it.