By geometry and volume first, load path second. Casting buys shape: internal cavities and complex bosses from one pour, and it tolerates a thick-to-thin transition a die cannot fill. Forging buys soundness and direction: closed grain flow following the load and more fatigue margin per kilogram. At one-off to low hundreds a pattern is cheap and a forging die is not; at tens of thousands it reverses.
Cost is tooling plus machining, spent differently by each route. A sand casting is dimensioned to the tolerance classes of ISO 8062, with a machining allowance you pay to remove. A close-die forging is bought to an EN 10250 class off a repeatable blank, usually with less metal to cut but with draft, fillet radii and a parting line the drawing has to accept. Neither route is cheaper in general - only for your quantity and your shop.
Defects are different families with different detection methods. Castings carry shrinkage porosity, gas porosity, inclusions, cold shuts, hot tears and misruns - which is why radiography to ISO 4993 or ultrasonic testing to an EN 12680 acceptance class belongs in a casting order. Forgings carry laps, internal bursts from aggressive upsetting, unfilled die corners and flash-line cracks, found mainly by magnetic particle testing and ultrasonic examination. Naming the defect you are protecting against is the fastest route decision.
The same part through both routes - what each buys and what it asks you to prove| Decision axis | Favour casting when | Favour forging when | The fact to put on the paper |
|---|
| Quantity and tooling | one-off to low hundreds, or the design is still moving | the volume repeats and the die cost amortises over the programme | annual volume, expected programme life, and who pays for the die if the drawing changes |
|---|
| Geometry | internal passages, hollow bosses, abrupt section changes, complex outer form | the load path is through the part and a parting line is acceptable | minimum section, draft angle, fillet radius and where the parting line may sit |
|---|
| Property direction | load is diffuse, the section is bulky, and the surface carries the stress | fatigue, impact or a notched path - grain flow can be oriented across it | the design stress, the safety factor, and where a crack would start |
|---|
| Section that can be worked | the core cannot be deformed by any press that could hold the die | the whole section actually strains, because the strength gain is a deformation effect | the working ratio, and whether the core saw any strain at all |
|---|
| Dimensional route | near-net shape with a machining allowance, tolerance class from the casting standard | close-die accuracy to an EN 10250 class, less metal removed | machining minutes per part and the datum scheme on the drawing |
|---|
| Soundness proof | volumetric inspection is available and the acceptance class is written into the order | surface methods plus ultrasonic, with a hardness traverse proving the heat treatment | which method, on which surface, at what acceptance level, on how many pieces |
|---|
| Consequence of a reject | a pattern fix is days, and one lost pouring is replaceable | a lap in a loaded fillet is a fatigue crack already born | the tooling lead time, not only the part lead time |
|---|
Values are the published minima, maxima or bands of the standards named in the table, taken at the stated thickness, size or temperature. Where a standard tabulates a value by size band, the value for your goods comes from the mill or test certificate, which we attach to the quotation instead of summarising it here.