Can an A2-70 stainless bolt replace A4-80, and which class should I actually order?

A4-80 is not an upgrade of A2-70; it is two changes at once. In ISO 3506 the letters name the alloy group and the number the strength: A2 is an 18 % chromium, 8 % nickel austenitic with no molybdenum, A4 the same family with 2-3 % molybdenum for pitting resistance. A2-70 is therefore 700 MPa of the cheaper alloy, A4-80 800 MPa of the corrosion-resistant one.

A4-80 is not an upgrade of A2-70; it is two changes at once. In ISO 3506 the letters name the alloy group and the number the strength: A2 is an 18 % chromium, 8 % nickel austenitic with no molybdenum, A4 the same family with 2-3 % molybdenum for pitting resistance. A2-70 is therefore 700 MPa of the cheaper alloy, A4-80 800 MPa of the corrosion-resistant one.

Austenitic bolting does not behave like 8.8 carbon steel. There is no clean yield point, so the joint is designed against a proof stress well below the tensile figure - about 450 MPa for class 70 and 600 MPa for class 80, falling further as diameter rises. Class 80 comes from cold work and is offered in a narrower diameter range than class 70. Elongation is generous, which is why an over-tightened stainless bolt necks without warning.

The third fact decides most orders: austenitic stainless galls. Threads seize after a few turns under load, and that seizure is friction welding rather than wear, so a torque spec written for plated steel is wrong. Assemble lubricated and at controlled speed, never re-use a galled fastener, and read the alloy choice against the environment: A4 for chloride splash and coastal air, and A2-70 into aluminium or carbon steel brings its own galvanic problem.

ISO 3506-1 designations - the letters are chemistry, the number is tensile class; proof stress and hardness bands are by diameter, from the standard table
DesignationAlloy familyMinimum tensileProof stress in practiceWhere it belongs
A2-70Austenitic 18 % Cr - 8 % Ni, no molybdenum (1.4301-type chemistry)700 MPaabout 450 MPa Rp0.2 in the smaller diameter bands, lower as diameter risesIndoors, dry or mild outdoor exposure; the default stainless bolt
A2-80Same group, more cold work800 MPaabout 600 MPa band by diameterHigh-preload small fasteners and cold-formed screws; limited diameter range
A4-70Austenitic Cr-Ni with 2-3 % Mo (1.4401 / 1.4408-type chemistry)700 MPaabout 450 MPa band by diameterCoastal structures, chemical splash, food plant, pool and desalination areas
A4-80Same alloy, cold worked to the higher class800 MPaabout 600 MPa band by diameterLoad-bearing marine and offshore fittings where A2 would pit
A2-50 / A4-50Solution-annealed or lightly worked condition500 MPaa few hundred MPa at most - the class table governsWhere formability, welding after installation or a lower clamp load matters more than preload
Ferritic and martensitic ISO 3506 groupsOther stainless families in the same standardNamed by the same hundreds-of-MPa logicMaterial and harder, with different corrosion behaviour and a magnetic responseSelf-tapping and hardness-driven applications, not chloride-exposed joints

Values are the published minima, maxima or bands of the standards named in the table, taken at the stated thickness, size or temperature. Where a standard tabulates a value by size band, the value for your goods comes from the mill or test certificate, which we attach to the quotation instead of summarising it here.

Where this costs money

Three situations where the difference becomes a claim

Each is a decision taken at quotation stage, while the specification is still cheap to change.

A coastal structure arrives specified A2

Within a couple of seasons the heads and the washers pit, and the rust staining is blamed on the bolt rather than on the alloy choice. Within reach of sea spray or de-icing salt, A4 is the group to order, and the detailing has to help it: no crevices under rubber washers, no dissimilar metal contact, and drain paths that do not hold chloride.

Someone swapped 8.8 for A2-70 because "700 is like 800"

The tensile figures are close, the proof stresses are not, and a designed preload joint depends on the proof stress. Substituting austenitic stainless into a joint calculated on carbon steel loses clamp force and lets the members separate or fret. Either redesign the preload or use a different fastener - do not read the two numbers as peers.

Stainless bolt, mild-steel nut

The female side is softer and it goes first: the tapped hole or the plated nut strips while the bolt comes out undamaged, which is how a failure gets misdiagnosed as bad material. Match groups across the joint, use a tapped hole in material that can carry the load or a proper threaded insert, and treat galvanic pairs as a design decision with washers or isolation.

Questions buyers ask before they commit the specification

Is A4 stronger than A2?

Not as a rule. Both groups are sold in class 50, 70 and 80, so A2-80 is stronger than A4-70. The letter tells you the chemistry and therefore the corrosion behaviour; the number tells you the minimum tensile class. Write both, in the right order, on the enquiry - "A4-70" or "A2-70" - and never "stainless 700 MPa".

Why did my stainless screws seize?

Austenitic stainless galls: asperities weld under pressure and tear the thread as you keep turning. It is worse at speed, with large fasteners and with mismatched hardness. Fit them at a controlled low rpm, use a lubricating torque control or anti-seize, keep the thread engagement generous so load is not carried by one or two turns, and throw away anything that has begun to seize rather than forcing it home.

Which is right for a cold store or a cryogenic application?

Austenitic stainless is normally the better family, because it keeps toughness at temperatures where carbon-steel fasteners become a design problem. A2 and A4 are both used well below freezing, so the low temperature is rarely the reason to move from A2 to A4 - chloride exposure is. Note the lubricant and the seal compound you choose, since those fail at low temperature before the bolt does.

How do you check a stainless fastener is really A4?

Hand-held XRF reads the molybdenum, which is the difference between the two groups and the cheapest confirmation available; we do it on receipt and record the result. Alongside it we take the EN 10204 3.1 certificate for the batch, check hardness against the class, and test to destruction on a sample where the joint is load-bearing. A marking on the head is a claim, not evidence.

Can you hot-dip galvanise a stainless fastener?

No, and that is not a workaround for a corrosion problem. Zinc will not metallurgically wet to the chromium oxide layer, so the coating is patchy and it does not buy the pitting resistance that molybdenum in the alloy buys. If the environment needs more protection than A4 gives, the honest answers are a higher-alloyed family or a redesign.

Fit this to a real part

Send the drawing and the answer comes back with your numbers

The quotation for fasteners & bolts repeats this comparison against your grade, dimension, tolerance and test package, and names any deviation before production starts.

Ask about this specificationFasteners & Bolts category hub

How we verify it

  • Grade and condition checked against the EN 10204 3.1 certificate and the heat marking.
  • Boundary dimensions, class, clearance or rating measured on the inspection sheet.
  • Deviations offered in writing before production, never discovered after shipment.

Trading and sourcing company based in northern Xingtai, Hebei, about 60 km south of the provincial capital. We buy across the industrial clusters of central and southern Hebei and reach the northern ones on scheduled factory runs; the supplier visits, benchmarking and pre-shipment inspection are ours, done in person. Not a factory. Multi-category, quoted from drawings, consolidated into one container and one document pack, and inspected before the balance is paid; every order starts as an RFQ.

Inspection and documents →

Written first reply within 1 working day; priced answer within 2-5 working days.