Xingtai, Hebei · Hebei industrial clusters

Specification reference · updated 29 September 2026

Which zinc coating protects my steel parts longest - electrodeposited, hot-dip galvanised or zinc flake?

Thickness decides it, and then the test endpoint. Zinc corrodes at a fairly steady rate in a given atmosphere, so 8 µm of electrodeposited zinc is not a thin version of a 70 µm hot-dip coating - it is roughly a decade less life. ISO 1461 tabulates hot-dip minimum thickness by base-material thickness, and ISO 9227 salt-spray hours measure something different from outdoor service because the chamber never dries.

Thickness decides it, and then the test endpoint. Zinc corrodes at a fairly steady rate in a given atmosphere, so 8 µm of electrodeposited zinc is not a thin version of a 70 µm hot-dip coating - it is roughly a decade less life. ISO 1461 tabulates hot-dip minimum thickness by base-material thickness, and ISO 9227 salt-spray hours measure something different from outdoor service because the chamber never dries.

The families differ in more than micrometres. Electrodeposited zinc is thin, bright and dimensionally faithful, and it drives hydrogen into the steel during plating - which is why a de-embrittlement bake is normal practice on high-strength fasteners. Hot dip is thick and metallurgically bonded, protects the thread root and the cut edge, and adds enough metal to change a fit. Zinc flake is a binder-bonded lamellar coating baked at roughly 300 °C, dimensionally thin, and free of plating hydrogen.

Then the number gets abused. Salt-spray hours are quoted to first white rust on one sheet and to first red rust on another, and those are years apart. White rust is zinc corrosion product and does not mean the steel is attacking; red rust means it is. Ask which endpoint, which area, which edge condition, and whether the parts were nested in a box for the test - the geometry decides more than the brochure admits.

Zinc coating families - what each standard governs and what the thickness buys; read thickness bands and test hours from the named standard, not from this row
Coating routeStandard that governs itTypical dry thicknessWhat the thickness buysThe catch
Electrodeposited zinc, with passivationISO 2081 and, for fasteners, ISO 4042; Fe/Zn thickness designationsabout 5-12 µm on small parts and fastenersEven coverage, tight dimensions, cheap; the passivation chemistry sets the white-rust hours more than the zinc doesHydrogen embrittlement on high-strength steel; no protection in a crevice; corners go thin
Electrodeposited zinc plus sealed topcoatSame plating standard with a declared sealerroughly 12-20 µm in buildSeveral times the bare-plating hours to red rust in the chamberSealers abrade in transit; stacked parts scuff off at the heads and corners first
Hot-dip galvanised fabricated articlesISO 1461 (coating) with ISO 14713 for design and useby base thickness - commonly the 70 µm local / 85 µm mean band for material 6 mm and over, lower bands for thinner stockEdge and crevice protection, and a life you can estimate from the zinc loss rate for the exposure categoryThreads shift, hollow sections need vent and drain holes, and sharp corners draw thin coating
Hot-dip galvanised fasteners and washersISO 4042 thinking plus the thread allowance logic of EN ISO 965-2tens of micrometres on the crests, size and process dependentReal corrosion life on a small part that cannot be hot-dipped as a fabricated assemblyThe mating nut must be tapped with the coating allowance or nothing runs down; torque scatter rises
Zinc flake (lamellar zinc) systemsOrdered to a declared in-house or customer specification; no single ISO governs the familyabout 5-15 µm, more in multi-layer buildsSeveral hundred chamber hours at a thinness that keeps the thread fit, with no plating hydrogenBake temperature caps it near 300 °C; weak cathodic throw into a crevice; ask for the chromium-free declaration in writing
Zinc-rich paint systemISO 12944 series for the system, ISO 8501-1 for the surface preparation gradea defined dry-film build across primer and topcoatDurability classes rated in the standard with hours bandsUseless without the stated preparation grade; the coating is decoration if the blast profile is not verified

Values are the published minima, maxima or bands of the standards named in the table, taken at the stated thickness, size or temperature. Where a standard tabulates a value by size band, the value for your goods comes from the mill or test certificate, which we attach to the quotation instead of summarising it here.

Where this costs money

Three situations where the difference becomes a claim

Each is a decision taken at quotation stage, while the specification is still cheap to change.

A 240-hour salt-spray claim is treated as 240 hours of life

ISO 9227 is an accelerated chamber with constant wetting, and it ranks coatings rather than predicting calendar life. Outdoor life comes from the corrosion category of the site (ISO 9223 puts us in C1 to C5 or CX) and the zinc loss rate for that category. Two parts with the same chamber result can differ by a decade on a coastal rack and in a dry indoor store.

Class 10.9 fasteners plated, then left before baking

Hydrogen absorbed during pickling and plating sits in the lattice and leaves slowly. A bolt that tightens fine can fail days or weeks later with no warning and no deformation, and the investigation always starts at the wrong end. Where the plating is unavoidable, the de-embrittlement bake and its delay after plating belong on the purchase order, with the time recorded.

Galvanised threads that will not assemble, and hollow frames that come out half empty

Hot dip adds coating to the thread flanks, so the internal side needs the allowance or an oversize tap - and a galvanised bolt in an unplated nut is the same problem in reverse. On tube and box sections, missing vent holes keep zinc out of the cavity and can turn the dip itself into an accident. Specify allowance, venting and drainage before the coating is quoted.

Questions buyers ask before they commit the specification

Is hot-dip always better than electroplating?

No, only thicker. Hot dip wins where the part is exposed outdoors, welded or cut at the edges, and where a few tens of micrometres do not disturb the fit. Electroplating wins where the dimension matters - threaded gauges, polished looks, thin sheet that would distort in the zinc pot - and where the assembly is indoors. Zinc flake earns its place on high-strength fasteners and where a bake is already part of the process.

What is white rust and is it a failure?

It is the voluminous corrosion product zinc forms when water sits on a fresh coating with no carbon dioxide supply, typical of parts packed wet or stored with no drainage. A light bloom is cosmetic and can be left; a flaking layer means the coating has been consumed and the substrate is next. Report it with photographs, the stacking and the storage condition, not only the word.

How do you check a coating on arrival?

Sample per delivery lot, measure dry thickness by the magnetic method on non-magnetic coatings over steel (ISO 2178), record the highest, lowest and mean readings, and check the corners and thread crests specifically because that is where a claim starts. Alongside that we take the declared salt-spray report for the batch and, where the customer requires it, arrange an independent chamber test.

Does a zinc flake coating replace galvanising for outdoor steelwork?

Not for long-life exposed structures, because it is thin and its sacrificial throw into a scratch or a crevice is limited. It is a strong answer on fasteners, clamps and small components where dimensional control, hydrogen avoidance and torque behaviour matter more than decade-scale coating life. Where the frame needs both, the honest route is hot dip on the frame and flake on the hardware.

Can you specify the coating on my drawing instead of leaving it to the shop?

That is the normal way we work. The drawing gets the process, the governing standard, the thickness class, the passivation or seal, the de-embrittlement requirement with its timing, the test method with its endpoint, and the vent and drain details on hollow parts. Then the inspection sheet has numbers on it and a deviation is visible before the container closes.

Fit this to a real part

Send the drawing and the answer comes back with your numbers

The quotation for steel products repeats this comparison against your grade, dimension, tolerance and test package, and names any deviation before production starts.

Ask about this specificationSteel Products category hub

How we verify it

  • Grade and condition checked against the EN 10204 3.1 certificate and the heat marking.
  • Boundary dimensions, class, clearance or rating measured on the inspection sheet.
  • Deviations offered in writing before production, never discovered after shipment.

Trading and sourcing company based in northern Xingtai, Hebei, about 60 km south of the provincial capital. We buy across the industrial clusters of central and southern Hebei and reach the northern ones on scheduled factory runs; the supplier visits, benchmarking and pre-shipment inspection are ours, done in person. Not a factory. Multi-category, quoted from drawings, consolidated into one container and one document pack, and inspected before the balance is paid; every order starts as an RFQ.

Inspection and documents →

Written first reply within 1 working day; priced answer within 2-5 working days.

Quote it against your part, not the chart

Send the drawing, the standard your engineer named and the quantity. We reply with the priced specification, the substitution we recommend and why, and the inspection plan that proves it.