Two separate decisions. The ring is chosen from a standard size series (ISO 3601-1, or AS 568 in the Americas), which fixes internal diameter and cross-section with tolerances. The groove is designed to ISO 3601-3 for your pressure. Material decides survival: NBR −30 to +100 °C, EPDM −40 to +150 °C, FKM −20 to +200 °C continuous, not peak.
Groove depth is the squeeze, and squeeze is what leaks. For a static radial groove the elastomer is typically compressed by roughly 15-25 % of its cross-section, with the gland filled no further than about 85-90 % so the ring cannot be crushed or extruded. Above roughly 10 MPa a back-up ring goes on the low-pressure side: PTFE, or an elastomer of 90 Shore A or harder.
Most field failures are not the size, they are the material. EPDM swells and destroys itself in mineral hydraulic oil and fuel, NBR hardens and cracks in steam and hot ozone, and FKM - which looks like the safe answer - is attacked by steam, ketones and amines. Send the medium, the temperature and the cycle, not only the gland drawing.
Elastomer families for moulded seals - continuous temperature and media picture| Elastomer (ISO 1629 code) | Continuous temperature | Strong against | Weak against | Typical hardness |
|---|
| NBR (nitrile) | −30 to +100 °C | Mineral oil, hydraulic fluid, grease, fuel oil | Ozone, steam, glycol brake fluid, ketones | 50-90 Shore A (70 standard) |
|---|
| HNBR (hydrogenated nitrile) | −40 to +150 °C | Hot oil, ozone, mechanical load, belts and rod seals | Strong acids, polar solvents | 60-90 Shore A |
|---|
| EPDM | −40 to +150 °C (short 175 °C) | Steam, hot water, glycol brake and coolant fluid, ozone | Mineral oil, fuel, aromatic solvents | 50-90 Shore A |
|---|
| VMQ (silicone) | −60 to +200 °C | Cold flexibility, weathering, wide temperature band | Abrasion, steam under pressure, oils and fuel, high compression set | 40-80 Shore A |
|---|
| FKM (fluoroelastomer) | −20 to +200 °C (some grades −30 °C) | Fuel including ethanol blends, aromatics, hot oil | Steam, ketones, amines | 60-90 Shore A |
|---|
| FFKM (perfluoroelastomer) | −15 to +250 °C | Aggressive chemical and solvent mixtures | Cost; some amine and steam regimes still attack | 65-95 Shore A |
|---|
Values are the published minima, maxima or bands of the standards named in the table, taken at the stated thickness, size or temperature. Where a standard tabulates a value by size band, the value for your goods comes from the mill or test certificate, which we attach to the quotation instead of summarising it here.